Shot peening is a cold-working process that bombards a finished metal surface with controlled round media to leave a layer of residual compressive stress, which improves resistance to fatigue, stress corrosion cracking and galling. Short answer: a peening callout names the specification (today usually SAE AMS2430), the areas to peen and to mask, the media, an Almen intensity range with its test strip letter, and the coverage; without intensity and coverage the process cannot be verified and is just blasting.

By Saola Manufacturing engineering team · Published · Updated

Blasting for appearance, with glass bead or other media, is covered in bead blasting vs sandblasting. This page is about peening as a fatigue treatment: what the numbers mean, which documents govern it, and how to put it on a drawing so that the result can be checked.

On this page

What does shot peening do to a machined part?

It plastically stretches a thin surface layer, which the material underneath holds back, so the surface ends up in compression. Fatigue cracks start at the surface under tension, and that compressive layer delays them.

MIL-S-13165C describes the purpose of peening as inducing residual compressive stresses in specified surfaces to improve resistance to fatigue, stress corrosion cracking and galling (MIL-S-13165C, Section 1.1). The same specification sets the order of work: all heat treatment, machining and grinding are completed before peening, fillets are formed, burrs are removed and edges to be peened get enough radius for complete coverage without distortion. Peening is therefore one of the last operations on the part, and the drawing has to reflect that.

Typical candidates are shafts with shoulders and fillets, springs, gears, connecting parts with cross holes, and welded or ground areas under cyclic load. The benefit depends on the material, the load and the process control, so the size of any fatigue improvement should come from your own test data or design code, not from a general rule.

What do Almen intensity and coverage mean?

Intensity is the energy of the shot stream, measured as the arc height of a standard steel test strip peened on one side; coverage is the share of the surface that has been dented. They are separate requirements and both go on the drawing.

Intensity is written as an arc height with the strip letter: per MIL-S-13165C, a specified intensity of 6A denotes an arc height of 0.006 to 0.009 in on the A strip, because a minimum-only intensity carries a tolerance of minus zero, plus 30 percent, but never less than 3 units. The N strip is for low intensities and the C strip for high ones, and the specification gives rough conversions between them (MIL-S-13165C, 3.3.6 and 6.10). Intensity is only valid at saturation: per MIL-S-13165C, doubling the exposure time of a strip at the saturation point should raise its arc height by no more than 10 percent, read from a saturation curve. SAE J442 defines the strips, holder and gage, and SAE J443 the procedure for using them; both have been revised since the editions linked here, so cite the current revision (SAE J443).

Coverage is checked on the part. MIL-S-13165C defines complete visual coverage as uniform and complete denting or obliteration of the original surface, examined with a ten-power glass, optionally with a liquid tracer that the peening removes. Per MIL-S-13165C, 6.14, critical applications and steels over 200,000 psi tensile strength may need additional peening time built into the process to make sure coverage is complete.

Default peening intensity (arc height range, inches, with test strip) when the drawing gives none · per MIL-S-13165C (1989), Table VI; specification canceled in 1998, shown for the values only. For steel over 200,000 psi the old specification required the intensity to be stated on the drawing.
Section thicknessSteel under 200,000 psiSteel over 200,000 psi; titaniumAluminum, metallic or ceramic shotAluminum, nonmetallic shot
Under 0.090 innot listednot listednot listed0.004–0.008 N
0.090 to 0.375 in0.008–0.012 A0.006–0.010 A0.006–0.010 A0.008–0.012 N
Over 0.375 in0.012–0.016 A0.006–0.010 A0.010–0.014 A0.012–0.016 N

Which shot peening specification should the drawing cite?

For new drawings, SAE AMS2430 is the general peening specification, with AMS2432 where computer-monitored peening is required (SAE AMS2432). MIL-S-13165C still appears on old drawings, but it was canceled and its line now ends in AMS2430.

SAE lists AMS2430V, revised in November 2026, as covering the requirements for shot peening of part surfaces by impingement of metallic, glass or ceramic shot; the 2009 withdrawal notice below still names it “Shot Peening, Automatic”, while the current title is simply “Shot Peening” (SAE AMS2430V). The Department of Defense canceled MIL-S-13165C in 1998 in favor of AMS-S-13165, and in 2009 withdrew its adoption of AMS-S-13165 because SAE superseded it with AMS2430 (MIL-S-13165C Notice 1; AMS-S-13165 withdrawal notice). If an old drawing calls MIL-S-13165C, ask the design owner whether AMS2430 is an acceptable replacement rather than quietly switching.

The AMS documents are paid; we do not quote their clause values here. Cite the specification with its revision letter or “latest revision”, and put the part-specific numbers (intensity, coverage, areas) on the drawing, because the specification's defaults may not suit your part.

How do you write the shot peening note on the drawing?

State the specification, the peened areas and masked areas on the view, the media type and size, the intensity range with strip letter, the coverage, and any limit on what may happen after peening.

A complete note usually reads like this, in words adapted to your part: “Shot peen areas marked P per AMS2430, cast steel shot, size per note, intensity range with strip letter, coverage complete or a stated multiple, mask threads and areas marked M, no machining after peening.” The items behind it:

  • Areas: mark the zones to peen and those that must be free of peening marks; MIL-S-13165C treats unmarked areas as optional and allows a boundary variation unless the drawing says otherwise.
  • Media: cast steel shot, cut wire, glass or ceramic beads, with a size. The old specification limited shot to no more than half the fillet radius in fillets and a quarter of the width of a slot the shot must pass through, which is a useful check on small features.
  • Intensity: a range, not a single value, with the strip letter (N, A or C), and the location on the part where it is verified.
  • Coverage: complete, or a multiple for critical parts, and the verification method (magnifier or tracer).
  • Sequence: magnetic particle or penetrant inspection before peening, and no operations after peening that remove or relieve the layer.

What is not allowed after a part has been shot peened?

Anything that removes the compressed layer or relieves it with heat. That rules out later machining or grinding of peened surfaces and limits the temperature of coating cures and embrittlement-relief bakes.

MIL-S-13165C prohibits operations after peening that relieve the peening stresses or create detrimental residual stresses, and caps post-peening heating, for example at 475 °F for steel parts (300 °F for steels tempered below that), 200 °F for aluminum alloys and 600 °F for titanium alloys (MIL-S-13165C, 3.3.10). It also notes that electroplated coatings applied after peening may put tensile stress on a steel surface. If the part is plated, painted or baked after peening, check the cure and bake temperatures against the limit in the specification you cite, and say on the drawing which operation comes first.

Peening also changes the surface: it leaves a dimpled texture, and per MIL-S-13165C, 6.6 peening very thin or small sections at high intensity can distort them. Hold tight dimensions on areas that are masked, and check flatness and thin walls after peening on the first article.

How is shot peening different from bead blasting for appearance?

Both throw media at the part, but peening is specified and accepted by intensity and coverage for a mechanical result, while cosmetic blasting is specified by appearance or roughness. A glass-bead finish note does not give you a peened part.

A blast finish note controls the look: media, a sample or a roughness range. A peening note controls a stress state that you cannot see, which is why it needs test strips, saturation curves and coverage checks, and records for each batch. Spherical, unbroken media matter for peening; MIL-S-13165C limits the share of deformed or broken shot in the machine and requires regular checks. If a part needs both a cosmetic finish and fatigue protection, call them as two separate requirements and state the order.

How do you accept shot-peened parts?

Ask for a peening certificate with the specification, media, Almen strip results against the specified range, saturation data, and coverage verification for the lot, then do a visual coverage check yourself.

The certificate should identify the parts and lot, the specification and revision, media type and size, the intensity measured on each strip with the strip letter and holder location, and the coverage method and result. On receipt, examine the peened areas with a ten-power magnifier for uniform denting, check that masked threads and faces are free of peening marks, and confirm that no machining marks cut through peened areas. For new parts, put these items in the first-article plan so the record exists from the start.

Can Saola supply machined parts that need shot peening?

Shot peening is not on our current finish menu, so a peening requirement must be raised at drawing review. The machining runs at our lead CNC plant.

Turned and milled parts are made at the lead CNC plant in Vietnam, described on the CNC turning and CNC milling pages. Finishes are a managed process with a fixed menu of eight on the surface finishing page, and shot peening is not one of them. If your drawing calls for peening, keep the full note on the drawing and flag it in the quote request; at drawing review we will tell you how that step can be handled for the part. First-article inspection reports for new parts and a dimensional inspection record per lot are available on request.

Frequently asked

What does 8-12A mean on a drawing?

It is an Almen intensity range: an arc height of 0.008 to 0.012 in measured on the A test strip at saturation. The letter matters; the same number on the N or C strip is a different intensity.

Who decides how long the part is peened?

The peener, from the saturation curve and the coverage checks. The drawing states the result (intensity range and coverage), and MIL-S-13165C made achieving full coverage the contractor's responsibility unless the order said otherwise.

Can aluminum parts be shot peened?

Yes. The old military table gives separate intensities for aluminum, and MIL-S-13165C asks for chemical cleaning of aluminum parts peened with steel shot to remove iron residue.

Does shot peening replace a better material or a larger fillet radius?

No. Peening adds margin to a sound design. Fix sharp corners, rough fillets and undersized sections first, then peen.

Should threads be shot peened?

Usually threads are masked, because peening can damage the flanks and the gauge fit. Rolled threads already carry compressive stress at the root; see rolled vs cut threads.

Sources

  1. MIL-S-13165C, Shot Peening of Metal Parts, U.S. Department of Defense, 1989 (Sections 1.1, 3.3, 6.10–6.14, Table VI)
  2. MIL-S-13165C Notice 1, cancellation, U.S. Department of Defense, 1998
  3. SAE-AMS-S-13165, withdrawal of adoption notice, U.S. Department of Defense, 2009
  4. AMS2430V, Shot Peening, SAE International, 2026
  5. AMS2432D, Shot Peening, Computer Monitored, SAE International, 2013 (later revision E, 2022)
  6. J443, Procedures for Using Standard Shot Peening Almen Test Strip, SAE International, 2017 revision (since revised)
  7. J442, Test Strip, Holder, and Gage for Shot Peening, SAE International, 2022 revision (since revised)

Have a drawing for this? Send it for a quote.

STEP or PDF, one part or a whole family. You get a unit price at your volume, the tooling cost, and a short manufacturability note.