Which aluminum anodizing colors hold up, and how do you call them out on a drawing?

Short answer

Aluminum anodizing colors are the shades you get by loading the porous oxide film of an anodized part with an organic dye, an inorganic dye or a metal deposited electrolytically, then sealing it. Short answer: black, clear, the bronzes and inorganic gold are the safest choices for repeat production and outdoor use, while bright reds, blues, purples and pale tints are possible but only hold up if you ask for an exterior-grade dye, a thick enough film and a good seal, and none of them will match across different alloys.

By Saola Manufacturing engineering team · Published · Updated

This guide is for design engineers and buyers choosing a color for a machined aluminum part. Lot-to-lot matching, limit samples and Delta E tolerances are covered in anodized color matching; this page is about the earlier decision: which color to pick, which coloring method sits behind it, and what to write so the finisher cannot hand you a dye that fades in the first summer.

On this page

Which anodizing colors are the most stable in production?

Clear, black, the bronze range and inorganic gold are the most forgiving colors, because they are either undyed or made with very stable colorants. Saturated reds, blues, greens and purples come from organic dyes and show every change in film thickness, dye bath condition and alloy.

The color of an anodized part is not a paint layer on top; it sits inside the pores of the oxide. The Aluminum Anodizers Council lists four ways to get it: electrolytic (two-step) coloring, where a metal salt such as tin, cobalt, nickel or copper is deposited at the base of the pores; integral coloring, which forms bronze and black shades during anodizing itself; organic dyeing, which gives the widest range of vivid colors; and interference coloring, which uses optical effects (AAC, Anodizing Definitions and Methods). Each method has a natural color range, and the process behind the color matters more than the color name on the drawing.

In practice, the colors that repeat best from lot to lot are the ones with the least dye in them. Clear anodize has none, so its only variable is the alloy and the film. Black is so dense that small drifts in dye uptake barely show. Bronze and black from the two-step electrolytic process are controlled by current and time, which is why architectural extrusions use them. The colors that drift most are mid-saturation organic shades such as a medium blue, a red or a light gold: a slightly thinner film holds less dye, and the eye picks up the difference immediately on parts mounted side by side.

That does not make bright colors a bad idea. It means a bright color needs a physical color standard, an agreed light source and a tolerance, which the color matching guide covers in detail.

Do anodized colors fade outdoors, and which ones fade first?

Some do. Fading is a property of the specific dye, the film thickness and the seal, not of the color name: an exterior-grade red can outlast an indoor-grade black.

Dye makers publish a light fastness number for each anodizing dye. For example, the maker's data sheets list an exterior-grade red at greater than 9 (Sanodal Red B3LW data sheet) and an exterior-grade turquoise at greater than 9 for applications up to architectural outdoor use (Sanodal Turquoise PLW data sheet). The same maker's deep black is rated greater than 8 at a 12 µm film and greater than 10 at a 25 µm film (Sanodal Deep Black H3LW data sheet), which shows how much the film thickness changes the result for the same dye.

Inorganic gold behaves differently again. The maker describes its iron-based gold as not a true organic dye but an iron compound that forms a colored complex with the oxide, and notes a known “first break”: a slight initial fade after short exposure that then stops (Sanodal Gold 4N data sheet). So a gold part can shift a little early on and then stay put.

The trap is that many finishers stock general-purpose dyes for indoor parts, which are cheaper and easier to run. If the drawing just says “red anodize”, nothing stops the finisher from using one. For any part that sees sunlight, the drawing or PO has to ask for an exterior-grade dye or a light fastness test result.

Color choice by service condition · light fastness test and dyed-coating requirements per MIL-A-8625F (1993); coloring methods per AAC (2026)
ColorUsual coloring methodIndoor partsOutdoor or UV-exposed parts
ClearUndyed (MIL-A-8625F Class 1)Low riskLow risk; alloy tint still shows
BlackOrganic dye, or electrolytic / integralLow riskAsk for exterior-grade dye or electrolytic black, plus a light fastness test
Bronze shadesElectrolytic (two-step) or integralLow riskLow risk; standard architectural choice
GoldInorganic (iron-based) or organic dyeEitherPrefer inorganic gold; expect a small early shift
Red, blue, green, purpleOrganic dye (Class 2)Works; needs color standardOnly with an exterior-grade dye named or tested; call out the light fastness test
Pale tints and pastelsOrganic dye at low strengthHardest to repeatHighest fade risk; avoid unless tested

How does the aluminum alloy change the anodized color?

The alloy sets the base tone under the dye, so the same dye on 6061, 7075, 2011 and cast aluminum gives four different shades. Pick one alloy per color-matched assembly, or accept a visible difference.

6061 is the usual reference alloy because it anodizes to a fairly neutral film. Copper-bearing alloys such as 2011 and 2024 and the zinc-rich 7075 give a darker, warmer or grayer film, so a dyed color comes out muddier, and high-silicon casting alloys anodize gray and blotchy. MIL-A-8625F reflects this: it requires the color on wrought alloys to be uniform but allows cast alloys to show dye bleed-out or lack of color uniformity, with the acceptable degree left to the buyer (MIL-A-8625F). The alloy-by-alloy detail, with composition limits, is in the color matching guide; for cast housings see anodizing die-cast aluminum.

The practical consequence: if a turned 2011 knob and a milled 6061 panel must look the same color, either change the knob to 6061 (if its machinability requirement allows), or put a note on both drawings that a shade difference between the two alloys is acceptable within an agreed limit sample. Do not discover the mismatch at assembly.

How do you call out an anodize color on the drawing?

Give the specification, type and class, then the color by name plus a physical reference, and only then the extras: exterior-grade dye, light fastness, seal and the surfaces that are cosmetic.

MIL-A-8625F splits coatings into Class 1 (non-dyed) and Class 2 (dyed), and for Class 2 it says the color and color uniformity requirements are whatever the contract, purchase order or drawing specifies (MIL-A-8625F, paragraphs 3.5, 3.6 and 3.6.1). It also recommends that dyed coatings preferably be Type II, because thinner Type I, IB, IC and IIB films are harder to dye, and it says black may not be readily obtainable on them. The specification lets you use FED-STD-595 chips only as an approximate guide, since those colors were written for paint.

A complete callout for a dyed decorative part reads like this:

  • Spec line: ANODIZE PER MIL-A-8625F, TYPE II, CLASS 2, COLOR: RED.
  • Color reference: MATCH APPROVED COLOR SAMPLE REF. [number]; LIGHT and DARK LIMIT SAMPLES GOVERN.
  • Outdoor parts: EXTERIOR-GRADE DYE REQUIRED; LIGHT FASTNESS TEST PER MIL-A-8625F PARA 4.5.4 REQUIRED ON FIRST LOT.
  • Cosmetic surfaces: identify them with a flag note so rack marks and contact points go elsewhere.

If you want a non-military reference instead, the Aluminum Association designation system used by the AAC builds the finish from mechanical, chemical and anodic codes, for example AA-M10 C22 A31 for a clear matte architectural finish (AAC, How to Specify Finishes on Aluminum). Either system works; mixing them on one drawing does not.

How do you test or accept light fastness on anodized parts?

Ask for it on the drawing: MIL-A-8625F has an optional light fastness test with a pass limit, but it only applies when the contract or drawing calls for it.

Per MIL-A-8625F, dyed (Class 2) specimens are exposed to ultraviolet light for 200 hours under ASTM G23, D822 or G26 without water spray, then compared with unexposed duplicates, and the color change must not exceed a Delta E of 3 measured per ASTM D2244 unless the contract sets another value (MIL-A-8625F, 3.7.1.3 and 4.5.4). The light fastness requirement is determined only when specified, so a drawing that is silent on it gets no test. The exposure apparatus named in a 1993 specification may not be what a finisher's lab runs today, so agree in writing which method and equipment will be used.

For a commercial part, a cheaper route is to ask the finisher to name the dye and send the dye maker's light fastness data, then run the full test once on the first lot only. Keep an unexposed sample from the approved lot sealed in a drawer: it is the reference you will need if a customer later complains that parts in the field have faded.

What should the RFQ say about anodize color?

State the color, the coloring method if you care, whether the part is indoor or outdoor, and who holds the master color sample. Those four facts decide the price and whether the color will repeat.

A short checklist for the RFQ or PO:

  • Alloy and temper for every part that must match (an alloy change later changes the color).
  • Color name plus the physical standard: a supplied sample, a previous approved part, or a sample to be made and approved before production.
  • Service: indoor, outdoor, or behind glass in sunlight. Outdoor means exterior-grade dye or electrolytic color.
  • Cosmetic surfaces and acceptable rack mark locations.
  • Whether a color difference between alloys or between machined and cast parts is acceptable.
  • Masked features (threads, bores, grounding points), because masking edges show on dyed parts.

If the part also has tight bores or threads, read anodizing dimensional change before fixing the film thickness; a thicker film for better light fastness also means more growth on every surface.

How does Saola handle colored anodizing on machined parts?

Machining runs at our lead CNC plant in Vietnam, and anodizing is one of the eight finishes on our managed finish menu, done at partner plants we manage. Color, dye grade and light fastness are agreed at drawing review, before any production lot.

Parts are machined on the CNC milling and turning lines at the lead plant, then sent to a partner finisher. Our surface finishing page lists the full finish menu. At drawing review we confirm the alloy for every part that must match, ask which color sample governs, and flag outdoor parts so the dye grade and any light fastness test are written into the order. If you need a color for which no sample exists yet, a sample is anodized and approved first. To start, send the drawing and color requirement through the quote form.

Frequently asked

Can anodized aluminum be any color?

A wide range of hues can be dyed, but not every hue is stable, and the film is translucent, so the metal and its surface prep always show through. If you need an opaque color that matches painted parts, powder coating is usually the better fit.

Is black anodize the most durable color?

Black is forgiving in production, but black dyes are not all equal, and the dye maker data above shows that even an exterior-grade black rates higher on a thicker film. See black anodize on aluminum for the outdoor options.

Can I use a Pantone or RAL number for an anodize color?

Use it as a description, not as the acceptance standard. Anodized color is translucent and metallic, so it never matches a printed or painted chip exactly. MIL-A-8625F treats even FED-STD-595 as an approximate guide only. The approved physical sample governs.

Does a thicker anodize film make the color last longer?

Generally yes, because a thicker film holds more dye; the dye maker data above shows a higher light fastness rating at the thicker film. The cost is more dimensional growth and a darker shade, so set the thickness on the drawing rather than leaving it to the finisher.

Why did my red parts come out pink on one lot?

Usually a thinner film, a weaker dye bath or a different alloy or etch. A limit sample on the PO turns that argument into a simple pass or fail at incoming inspection.

Sources

  1. MIL-A-8625F, Anodic Coatings for Aluminum and Aluminum Alloys, U.S. Department of Defense, 1993 (paragraphs 3.5, 3.6, 3.7.1.3, 4.5.4, 6.6, 6.12)
  2. Anodizing Definitions and Methods, Aluminum Anodizers Council, accessed 2026
  3. How to Specify Finishes on Aluminum, Aluminum Anodizers Council, accessed 2026
  4. Sanodal Red B3LW product data, Heubach, accessed 2026
  5. Sanodal Turquoise PLW Liq product data, Heubach, accessed 2026
  6. Sanodal Deep Black H3LW product data, Heubach, accessed 2026
  7. Sanodal Gold 4N product data, Heubach, accessed 2026

Have a drawing for this? Send it for a quote.

STEP or PDF, one part or a whole family. You get a unit price at your volume, the tooling cost, and a short manufacturability note.